LOCTITE EA 9628

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EA 9628 060NW Aero

Main features

  • Toughened Structural Bonding
  • Knitted or Non-Woven Nylon Carrier
  • Lap-Shear, Peel, and Environmental Performance

Product Description

LOCTITE EA 9628 AERO is a modified epoxy film adhesive for structural bonds requiring toughness. It is supplied ready to use with either a knitted nylon carrier as LOCTITE EA 9628K AERO or a non-woven nylon mat as LOCTITE EA 9628NW AERO. The adhesive uses a 235–250°F (113–121°C) heat-cure process and develops temperature-dependent lap shear and peel performance on prepared aluminum. Environmental-exposure testing includes water, humidity, hydraulic oil, JP-4 jet fuel, salt spray, and anti-icing fluid under the documented conditions.

Key features

  • Toughened structural film: Modified epoxy construction supports structural bonding applications requiring toughness and durability.
  • Two carrier options: Available with knitted nylon or non-woven nylon reinforcement to support different film constructions and cure schedules.
  • Elevated-temperature cure: Cures for 1 hour at 250°F (121°C) or 90 minutes at 235°F (113°C).

Applications / Suitable for

  • Structural bonded assemblies requiring toughness
  • Bonding prepared aluminum adherends
  • Metal-to-metal bonded structures
  • Aluminum honeycomb sandwich constructions

Technical Specifications

Mechanical Properties
Elongation
Elongation is the process of lengthening something. It is a percentage that measures the initial, unstressed, length compared to the length of the material right before it breaks. It is commonly referred to as Ultimate Elongation or Tensile Elongation at break.
7.5 %

Additional Information

Technical properties

As-supplied / before-processing properties

Product form, carrier options, storage requirements and documented assembly and cure parameters.

Property Value Unit Method or condition
Adhesive type Modified epoxy film adhesive — As supplied
Product form Ready-to-use adhesive film with protective liner(s) — Liner must be removed before assembly
Knit-supported variant LOCTITE EA 9628K AERO — Knitted nylon carrier fabric
Non-woven-supported variant LOCTITE EA 9628NW AERO — Non-woven nylon mat carrier
Film weight used for lap-shear testing 0.060 / 293 psf / g/m² ASTM D1002 test specimens
Storage temperature 0 / −18 or below °F / °C Refrigerated storage in sealed containers for maximum storage life
Warranty life 12 months From date of shipment when stored at 0°F (−18°C)
Open assembly time at 77°F (25°C) At least 20 days After removal from cold storage
Open assembly time at 90°F (32°C) At least 10 days After removal from cold storage
Recommended mating pressure 25–50 / 170–340 psi / kPa Typical pressure sufficient to assure proper mating
Primary cure schedule 1 hour at 250 / 121 °F / °C Pressure applied before heating and maintained through assembly cooldown
Alternative cure schedule 90 minutes at 235 / 113 °F / °C Pressure applied before heating and maintained through assembly cooldown
Heat-up rate 4–7 / 2.2–4 °F/min / °C/min Recommended rate to cure temperature
Technical properties

After-processing / final-state properties

Typical cured adhesive, bonded-joint and honeycomb-sandwich results. Values remain specific to the listed carrier, cure schedule, adherends, exposure and test conditions.

Property Value Unit Method or condition
Lap shear strength, −67°F (−55°C) Knit: 5,500 / 37.9; Non-woven: 5,500 / 37.9 psi / MPa ASTM D1002; 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933; knit cured 1 h at 250°F (121°C); non-woven cured 1.5 h at 235°F (113°C)
Lap shear strength, 77°F (25°C) Knit: 6,000 / 41.3; Non-woven: 5,800 / 40.0 psi / MPa ASTM D1002; same adherends and cure conditions
Lap shear strength, 180°F (82°C) Knit: 4,000 / 27.6; Non-woven: not reported psi / MPa ASTM D1002; same adherends and cure conditions
Lap shear strength, 250°F (121°C) Knit: 1,900 / 13.1; Non-woven: 2,100 / 14.5 psi / MPa ASTM D1002; same adherends and cure conditions
Lap shear after control conditioning Knit: 6,300 / 43.4; Non-woven: 6,300 / 43.4 psi / MPa Tested at 75°F (25°C); control at 77°F (25°C); ASTM D1002 specimen system and documented cure schedules
Lap shear after water exposure Knit: 6,300 / 43.4; Non-woven: 6,300 / 43.4 psi / MPa 30 days in water at 77°F (25°C); tested at 75°F (25°C)
Lap shear after humidity exposure Knit: 5,900 / 40.7; Non-woven: 5,900 / 40.7 psi / MPa 30 days at 120°F (49°C), 100% RH; tested at 75°F (25°C)
Lap shear after hydraulic-oil exposure Knit: 6,500 / 44.8; Non-woven: not reported psi / MPa 7 days at 77°F (25°C); tested at 75°F (25°C)
Lap shear after JP-4 jet-fuel exposure Knit: 6,100 / 42.0; Non-woven: 6,100 / 42.0 psi / MPa 7 days at 77°F (25°C); tested at 75°F (25°C)
Lap shear after salt-spray exposure Knit: 6,100 / 42.0; Non-woven: 6,100 / 42.0 psi / MPa 30 days at 105°F (41°C); tested at 75°F (25°C)
Lap shear after anti-icing-fluid exposure Knit: 6,300 / 43.4; Non-woven: 6,300 / 43.4 psi / MPa 7 days at 77°F (25°C); tested at 75°F (25°C)
T-peel strength, −67°F (−55°C) 28 / 125 lb/in / N/25 mm ASTM D1876; knit support cured 1 h at 250°F (121°C); 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933
T-peel strength, 77°F (25°C) 37 / 165 lb/in / N/25 mm ASTM D1876; knit support; same cure and adherend preparation
T-peel strength, 180°F (82°C) 34 / 151 lb/in / N/25 mm ASTM D1876; knit support; same cure and adherend preparation
Metal-to-metal climbing drum peel, −67°F (−55°C) Knit: 50 / 222; Non-woven: 45 / 200 in·lb/in / N/25 mm ASTM D1781; prepared 2024-T3 AlClad aluminum; documented variant cure schedules
Metal-to-metal climbing drum peel, 77°F (25°C) Knit: 70 / 311; Non-woven: 65 / 289 in·lb/in / N/25 mm ASTM D1781; same adherends and cure conditions
Metal-to-metal climbing drum peel, 180°F (82°C) Knit: 60 / 267; Non-woven: 55 / 245 in·lb/in / N/25 mm ASTM D1781; same adherends and cure conditions
Crack extension, Glc Knit: 8 / 1,401; Non-woven: 14.3 / 2,504 lb/in / N/m ASTM D3433; documented variant cure schedules
Crack extension, Gla Knit: 6 / 1,051; Non-woven: 10.4 / 1,821 lb/in / N/m ASTM D3433; documented variant cure schedules
Crack extension, Glscc after 5 weeks Knit: not reported; Non-woven: 6.1 / 1,068 lb/in / N/m ASTM D3433
Crack extension, Glscc after 15 weeks Knit: not reported; Non-woven: 4.0 / 700 lb/in / N/m ASTM D3433
Honeycomb climbing drum peel, −67°F (−55°C) Knit: 54 / 80; Non-woven: 45 / 67 in·lb/3 in / mN/m 2024-T3 clad aluminum with 0.25 in (6.35 mm) cell 5052 non-perforated aluminum core
Honeycomb climbing drum peel, 77°F (25°C) Knit: 60 / 89; Non-woven: 63 / 93 in·lb/3 in / mN/m Same honeycomb construction and documented variant cure schedules
Honeycomb climbing drum peel, 180°F (82°C) Knit: 48 / 71; Non-woven: 45 / 67 in·lb/3 in / mN/m Same honeycomb construction and documented variant cure schedules
Honeycomb flatwise tension strength, 77°F (25°C) Knit: 1,400 / 9.6; Non-woven: 1,300 / 8.9 psi / MPa 2024-T3 clad aluminum with 0.25 in (6.35 mm) cell 5052 non-perforated aluminum core
Approximate service temperature 250 / 121 °F / °C Defined as the temperature at which the adhesive retains 1,000 psi (6.9 MPa) by ASTM D1002
Bulk-resin tensile strength 7,500 / 51.7 psi / MPa ASTM D638; 0.125 in (3.18 mm) casting; tested at 77°F (25°C)
Bulk-resin tensile modulus 345 / 2,377 ksi / MPa ASTM D638; 0.125 in (3.18 mm) casting; tested at 77°F (25°C)
Elongation at break 7.5 % ASTM D638; 0.125 in (3.18 mm) casting; tested at 77°F (25°C)
Hardness 83 Shore D Tested at 77°F (25°C)
Glass-transition temperature, dry 248 / 120 °F / °C Tan delta by DMTA
Glass-transition temperature, wet 210 / 99 °F / °C Tan delta by DMTA
Shear modulus, dry 90.5 / 624 ksi / MPa DMTA; tested at 77°F (25°C)
Bulk-resin compressive strength 11,500 / 79.3 psi / MPa ASTM D695; 0.125 in (3.18 mm) casting; tested at 77°F (25°C)
Bulk-resin compressive modulus 310 / 2,136 ksi / MPa ASTM D695; 0.125 in (3.18 mm) casting; tested at 77°F (25°C)
Dielectric constant 3.56 — ASTM D150; 1 kHz
Dissipation factor 0.087 — ASTM D150; 1 kHz
Dielectric strength >258 V/mil ASTM D149

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers